管狀焊絲 | 焊劑 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | Mo | Mn | Fe | W | Ni | V | B | 其他 | Delcrome 103 | 107 | 54 | 5.15 | 27.50 | 1.50 | | 2.50 | Bal | | | | | | 磨煤輥 | Multipass 104 | 431 | 28 | 0.25 | 1.20 | 1.50 | | 3.00 | Bal | | | | | | 軋輥等堆焊過渡層及軸的修復(fù) | Multipass 105 | 431 | 45 | 0.50 | 4.00 | 1.10 | 0.50 | 2.75 | Bal | | | | | | 拖拉機(jī)惰輪、礦車輪、導(dǎo)輥 | Multipass 107 | 431 | 37 | 0.35 | 2.70 | 1.20 | 0.25 | 2.70 | Bal | | | | | | 卷筒、拖拉機(jī)惰輪、礦車輪 | Multipass 109 | 260 | | 0.45 | 3.10 | 0.60 | | 0.60 | Bal | | 0.5 | | | | 管模、鋁軋輥等 | Multipass 224 | 107 | 46 | 0.45 | 5.50 | 0.65 | 1.10 | 1.80 | Bal | 1.50 | | | | | 各類軋輥及連鑄第3區(qū)輥 | Multipass 224H | 107 | 53 | 0.55 | 6.50 | 0.65 | 1.10 | 1.80 | Bal | 1.50 | | | | 1.0 | 熱軋工作輥、支撐輥、開坯輥 | Multipass 224HC | 107 | 58 | 0.75 | 7.70 | 0.75 | 1.80 | 1.70 | Bal | 2.60 | | | | 1.0 | 支撐輥、校直輥、助卷輥 | Multipass 225 | 107 | 59 | 0.90 | 6.00 | 0.50 | 1.20 | 0.80 | Bal | 8.60 | | | | | 熱軋支撐輥 | Multipass 235 | 107 | 60 | 0.45 | 9.00 | | 2.20 | 0.70 | Bal | 8.40 | Co:10.5 | 0.30 | | | 熱軋支撐輥 | Multipass 236 | | | 0.28 | 3.10 | 0.70 | 2.00 | 0.70 | Bal | 1.90 | | 0.65 | | | 鋼管成型輥 | Multipass 915 | 107 | 60 | 1.20 | 20.00 | 0.50 | | 0.70 | Bal | | | | 4.00 | | 高速磨打擊板等耐強(qiáng)沖擊,強(qiáng)磨粒磨損場(chǎng)合 | Delstain 414-S | 260 | 40 | 0.20 | 14.00 | 0.50 | 1.00 | 1.40 | Bal | | 4.20 | | | | 連鑄輥等耐磨耐高溫場(chǎng)合 | Delstain 420 | 260 | 46 | 0.40 | 13.00 | 0.50 | | 1.40 | Bal | | | | | | 一般軋鋼輥、剎車鼓、卷輥 | Delstain 423 | 107 | 45 | 0.33 | 13.50 | 0.50 | 1.20 | 1.50 | Bal | | 2.50 | 0.20 | | | 連鑄機(jī)輥、熱軋輥堆焊 | Delstain 424H | 260 | 49 | 0.40 | 12.00 | 0.50 | 0.90 | 2.20 | Bal | | 1.40 | | | | 有色工作輥的堆焊 | Delstain 430 | 260 | | 0.10 | 19.00 | 0.50 | | 0.70 | Bal | | 0.60 | | | | 連鑄輥等耐磨耐高溫場(chǎng)合 | Delcrome 911 | 107 | 57 | 6.60 | 36.50 | 0.40 | | 0.40 | Bal | | | | | | 磨煤輥堆焊 | Delcrome 100HD | 107 | 57 | 6.80 | 29.00 | 1.00 | | 2.0 | Bal | | | | | Zr:0.45 | 磨煤輥等耐中等沖擊,強(qiáng)磨粒磨損場(chǎng)合 | STW 101 | 431 | HB:250 | 0.25 | 1.35 | 0.55 | 0.60 | 1.35 | Bal | | | 0.25 | | | 碳鋼、低合金鋼部件修復(fù) | STW 102 | 431 | 36 | 0.25 | 2.95 | 0.55 | 1.00 | 1.00 | Bal | | 1.35 | 0.10 | | | 碳鋼、低合金鋼部件修復(fù) | STW 103 | | | 0.35 | 3.00 | 0.70 | 2.00 | 1.40 | Bal | | | 0.60 | | | 碳鋼、低合金鋼部件修復(fù) | Stellite706司太立焊絲,Stellite706司太立焊絲, 2。(e)一個(gè)字母,焊條種類。, 焊條 - 藥皮, (3)藥皮類型:鈦鈣型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含氧化鈦30%以上,鈣、鎂的碳酸鹽20%以下,焊條工藝性能良好,熔渣流動(dòng)性好,熔深一般,電弧穩(wěn)定,焊縫美觀,脫渣方便,適用于全位置焊接,如j422即屬此類型,是目前碳鋼焊條中使用最廣泛的一種焊條。, (船用焊條除外), , , , , 六、藥皮在焊接過程中起著極為重要的作用。若采用無藥皮的光焊條焊接,則在焊接過程中,空氣中的氧和氮會(huì)大量侵入熔化金屬,將金屬鐵和有益元素碳、硅、錳等氧化和氮化形成各種氧化物和氮化物,并殘留在焊縫中,造成焊縫夾渣或裂紋。而熔入熔池中的氣體可能使焊縫產(chǎn)生大量氣孔,這些因素都能使焊縫的機(jī)械性能(強(qiáng)度、沖擊值等)大大降低,同時(shí)使焊縫變脆。此外采用光焊條焊接,電弧很不穩(wěn)定,飛濺嚴(yán)重,焊縫成形很差。, , 以結(jié)構(gòu)鋼為例:牌號(hào),編制法。結(jié)xxx,結(jié)為結(jié)構(gòu)鋼焊條,第3個(gè)數(shù)字,代表藥皮類型,焊接電流要求,第1、2數(shù):代表焊縫金屬抗拉強(qiáng)度 。, 3)硅(si )硅也是一種較好的合金劑,在鋼中加入適量的硅能提高鋼的屈服強(qiáng)度、彈性及抗酸性能;若含量過高,則降低塑性和韌性。在焊接過程中,硅也具有較好的脫氧能力,與氧形成二氧化硅,但它會(huì)提高渣的粘度,易促進(jìn)非金屬夾雜物生成。, , , , 管狀焊絲 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | Tungsmooth 60 | A-91 | 60%碳化鎢、其余為鋼管、A-91中的91為碳化鎢顆粒硬度 | 風(fēng)機(jī)攪拌機(jī)葉片、采礦、建筑易損件 | 管狀焊絲 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | Mo | Mn | Fe | Ni | Al | 其他 | Delcrome 11-o | 50 | 3.20 | 14.50 | 0.90 | 0.45 | 1.40 | Bal | | | | 破碎機(jī)錘頭、挖土機(jī)齒 | Delcrome 94-o | 57 | 3.20 | 24.50 | 0.70 | | 0.80 | Bal | 2.80 | | | 筑路機(jī)零件、攪拌葉片 | Delcrome 100-o | 57 | 3.80 | 26.50 | 1.40 | 1.30 | 1.90 | Bal | | | | 磨煤輥 | Delcrome 100HC-o | 60 | 5.50 | 26.50 | 2.40 | 1.30 | 1.90 | Bal | | | | 磨煤輥、破碎輥 | Delcrome 117-o | 43 | 2.30 | 10.50 | 1.30 | 1.50 | 1.50 | Bal | zr:0.40 | | Cu:0.40 | 破碎輥、錘頭 | Delcrome 150-o | 58 | 2.20 | 7.00 | | 2.00 | 1.00 | Bal | V:0.20 | | Ti:7.00 | 水泥擠壓輥、錘頭、農(nóng)具 | Delcrome 945-o | 57 | 5.00 | 21.50 | 0.70 | 4.50 | 0.70 | Bal | W:2.00 | | Nb:7.00 | 高爐加料槽板、閘閥 | Build up | 35 | 0.15 | 0.90 | 0.90 | 0.40 | 1.80 | Bal | | | | 碳鋼、低合金鋼恢復(fù)尺寸如齒輪、錘頭 | Ni-Mang-o | 冷硬 | 0.85 | 3.00 | 0.50 | | 14.00 | Bal | 3.00 | | | 破碎機(jī)輥、顎板、挖泥機(jī)刀片 | Sta-Mang-o | 冷硬 | 0.10 | 10.00 | 0.50 | 0.80 | 15.50 | Bal | 0.85 | | | 破碎機(jī)、鐵鏟、鐵路道岔 | Multipass 4-o | 34 | 0.15 | 0.70 | 1.10 | 0.30 | 2.00 | Bal | | | | 碳鋼、低合金鋼部件修復(fù) | Multipass 5-o | 44 | 0.10 | 2.30 | 0.30 | 0.50 | 1.40 | Bal | | | | 拖拉機(jī)惰輪、起重機(jī)輪 | Multipass 1265-g | 55 | 0.65 | 5.50 | 0.50 | 1.50 | 1.00 | Bal | W:1.50 | | V:0.30 | 冷沖壓模 | Delcrome 90G | 48 | 2.40 | 24.00 | 0.60 | | 0.90 | Bal | | | | 鏟斗齒、排氣葉、提升斗 | Delcrome 94G | 52 | 3.00 | 28.00 | 1.40 | | 1.20 | Bal | B:0.80 | | | 鏟斗齒、攪拌機(jī)、破碎輥 | Mulitpass 106 | | 0.10 | | 0.90 | 5.20 | 1.40 | Bal | 5.20 | | | 管模,鋁軋輥等 | Delcrome 165 | 62 | 6.80 | 30.00 | 3.00 | 0.50 | 0.50 | Bal | W:4.20 | | Nb:2.60 | 磨煤 輥等耐中等沖擊,強(qiáng)磨粒磨損場(chǎng)合 | Delstain 414N-o | 47 | 0.20 | 14.00 | 0.50 | 1.00 | 1.30 | Bal | 4.20 | | N:0.22 | 連鑄輥等耐磨耐高溫場(chǎng)合 | Delstain 431 | 33 | 0.40 | 17.50 | 0.50 | | 1.20 | Bal | | | | 連鑄輥等耐磨耐高溫場(chǎng)合 | Delcrome 103HD | 60 | 5.60 | 30.00 | 1.10 | 0.80 | 1.20 | Bal | | | Cu:0.10 | 磨煤輥等 | Stellarc 420 | 430(HV) | 0.3 | 13 | 1 | | 1 | Bal | | | | 具有一定的耐大氣腐蝕及良好的耐磨性,可用于一般機(jī)械零件的修復(fù)、保護(hù) | Stellarc 430 | 400(HV) | 0.7 | 17 | 1 | 0.5 | 1 | Bal | | | | 具有一定的耐大氣腐蝕及良好的耐磨性,可用于一般機(jī)械零件的修復(fù)、保護(hù) | Stellarc 316 | 240(HV) | 0.08 | 18 | 0.7 | 2.5 | 1 | Bal | 13 | | | 具有一定的耐大氣腐蝕及良好的耐磨性,可用于一般機(jī)械零件的修復(fù)、保護(hù) | Stellarc 100 | 660(HV) | 5 | 28 | 0.5 | | 1 | Bal | | | | 具有優(yōu)良的耐磨性 | Stellarc 250 | | | 1 | 0.5 | 0.5 | 1 | Bal | | | WC:50 | 風(fēng)機(jī)、風(fēng)管、煙道內(nèi)壁 | Stellarc 45 | 400(HV) | | 45 | | | | | Bal | | | 風(fēng)機(jī)、風(fēng)管、煙道內(nèi)壁 | Stellarc 95 | 480(HV) | | | | | | | Bal | 5 | | 打底涂層 | Stellarc 625 | 260(HV) | 0.08 | 21 | | 9 | | 5 | Bal | 5 | Nb+Ta:4 | 優(yōu)異的抗高溫腐蝕及耐磨介質(zhì) | Stellarc 276 | | 0.08 | 16 | | 16 | | 5 | Bal | | W:4 | 耐腐蝕性能優(yōu)異,能抗硫酸、鹽酸或其他有機(jī)酸的腐蝕 | Stellite706司太立焊絲,Stellite706司太立焊絲, , , , 此外,對(duì)于藥皮中含有多量鐵粉的焊條,可以稱為鐵粉焊條。這時(shí),按照相應(yīng)焊條藥皮的主要成分,又可分為鐵粉鈦型、鐵粉鈦鐵礦型、鐵粉氧化鐵型、鐵粉低氫型等,構(gòu)成了鐵粉焊條系列。, , , 5)鎳(ni)鎳對(duì)鋼的韌性有比較顯著的效果,一般低溫沖擊值要求較高時(shí),適當(dāng)摻入一些鎳。, , (9)藥皮類型:鐵粉低氫型 ‖藥皮主要成分 :鈣、鎂的碳酸鹽、螢石和鐵粉 ‖焊接電源:直流或交流, , (11)藥皮類型:鹽基型 ‖藥皮主要成分 :氯化物和氟化物 ‖焊接電源:直流, , , , 二、保護(hù)焊接熔池。焊接過程中,空氣中的氧、氮及水蒸氣浸入焊縫,會(huì)給焊縫帶來不利的影響。不僅形成氣孔,而且還會(huì)降低焊縫的機(jī)械性能,甚至導(dǎo)致裂紋。而焊條藥皮熔化后,產(chǎn)生的大量氣體籠罩著電弧和熔池,會(huì)減少熔化的金屬和空氣的相互作用。焊縫冷卻時(shí),熔化后的藥皮形成一層熔渣,覆蓋在焊縫表面,保護(hù)焊縫金屬并使之緩慢冷卻、減少產(chǎn)生氣孔的可能性。, 電焊條 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | W | Fe | Mo | Ni | Co | Mn | B | Cu | 其他 | Stellite 1 | 48 | 2.20 | 29.00 | 2.00 | 14.00 | 3.00 | 0.50 | 3.00 | Bal | 1.00 | | | | 閥座、軸承、刀口等 | Stellite 6 | 40 | 1.00 | 29.00 | 1.00 | 4.50 | 3.00 | 0.50 | 3.00 | Bal | 1.00 | | | | 發(fā)動(dòng)機(jī)氣門、高溫高壓閥門、渦輪機(jī)葉片 | Stellite 12 | 44 | 1.30 | 29.00 | 1.00 | 9.00 | 3.00 | 0.50 | 3.00 | Bal | 1.00 | | | | 高溫高壓閥門、鋸齒、螺旋推桿等 | Stellite 21 | 23 | 0.30 | 28.00 | 1.00 | | 2.50 | 5.50 | 2.50 | Bal | 2.00 | | | | 渦輪機(jī)葉片、閥座、熱沖模 | Stellite 25 | 冷硬 | 0.15 | 20.00 | 1.00 | 14.00 | 3.00 | 0.50 | 10.00 | Bal | 1.50 | | | | 高溫耐蝕密封面、擠壓模 | Nistelle C | | 0.10 | 17.00 | | 5.00 | 6.00 | 17.00 | Bal | | | | | | 高溫耐蝕密封環(huán) | Ni-Mang | 冷硬 | 0.60 | 2.70 | 0.20 | | Bal | | 3.70 | | 13.50 | | | | 錘式破碎機(jī)、高錳鋼部件焊接 | STE 308-16 | | 0.08 | 19.50 | 0.90 | | Bal | 0.50 | 10.00 | | 0.80 | | 0.50 | | 用于焊接Cr18Ni8不銹鋼 | STE 308L-16 | | 0.03 | 19.50 | 0.90 | | Bal | 0.50 | 10.00 | | 0.80 | | 0.50 | | 用于焊接超低碳Cr18Ni8不銹鋼 | STE 309-16 | | 0.15 | 23.50 | 0.90 | | Bal | 0.50 | 13.00 | | 0.80 | | 0.50 | | 用于焊接Cr22Nil2不銹鋼及用于不銹鋼與低碳鋼或低合金鋼之間的焊接 | STE 309L-16 | | 0.02 | 23.50 | 0.90 | | Bal | 0.50 | 13.00 | | 0.80 | | 0.50 | | 打底層焊接,異種鋼焊接,易產(chǎn)生裂紋部位的焊接 | STE 309Mo-16 | | 0.12 | 23.50 | 0.90 | | Bal | 2.50 | 13.00 | | 0.80 | | | | 用于焊接Cr22Nil2-Mo不銹鋼 | STE 309MoL-16 | | 0.03 | 23.50 | 0.90 | | Bal | 2.50 | 13.00 | | 0.80 | | | | 用于焊接超低碳Cr22Nil2Mo不銹鋼 | STE 310-16 | | 0.20 | 26.50 | 0.75 | | Bal | 0.50 | 21.50 | | 1.50 | | 0.50 | | 用于焊接Cr25Ni20不銹鋼 | STE 310Mo-16 | | 0.08 | 26.50 | 0.75 | | Bal | 2.50 | 21.00 | | 1.20 | | 0.50 | | 耐硫酸腐蝕、抗裂性、高溫性能優(yōu)良 | STE 316-16 | | 0.05 | 18.50 | 0.90 | | Bal | 2.50 | 12.50 | | 0.80 | | 0.50 | | 用于焊接Cr18Ni12Mo2不銹鋼 | STE 316L-16 | | 0.03 | 18.50 | 0.90 | | Bal | 2.50 | 12.50 | | 0.80 | | 0.50 | | 用于焊接超低碳Cr18Ni12Mo2不銹鋼 | STE 316LF | | 0.02 | 18.00 | 0.75 | | Bal | 2.70 | 16.00 | | 2.00 | | 0.50 | | 耐尿素腐蝕性優(yōu)良 | STE 347-16 | | 0.08 | 19.50 | 0.50 | | Bal | 0.50 | 10.00 | | 0.80 | | 0.50 | 8xc-1.00 | 用于焊接Cr18Ni8含鈮或鈦的不銹鋼 | STE 997 | 56 | 0.60 | 5.50 | 0.80 | | Bal | 4.00 | W:7.0 | | 0.70 | | | | 低氫型高速鋼焊條 | D 287 | 40 | 0.10 | 14.00 | 0.50 | | Bal | 1.00 | 5.00 | | 0.50 | | | | 水泵、水輪機(jī)部件 | D 907 | 冷硬 | 0.20 | 21.00 | 1.00 | 2.50 | Bal | 3.00 | | 20.00 | 1.50 | | | | 熱剪刀片 | Delcrome 90sc | 52 | 2.10 | 26.00 | 1.10 | | Bal | | | | 0.90 | | | | 挖掘設(shè)備、破碎輥、錘 | Delcrome 91 | 55 | 3.00 | 31.00 | 0.60 | | Bal | 1.30 | | | 0.90 | | | | 破碎機(jī)輥、錘頭、泥漿泵部件 | Delcrome 94 | 53 | 3.00 | 31.00 | 0.40 | | Bal | 1.30 | | | 0.90 | | | | 鏟斗齒、攪拌機(jī)、挖掘采礦設(shè)備 | Delcrome 945 | 58 | 5.40 | 1.20 | | Bal | | | | 1.00 | | | Nb:5.00 | 耐侵蝕、抗高溫腐蝕及磨損場(chǎng)合 | Delcrome 23 | 44 | 0.20 | 5.50 | 1.00 | &n, bsp;&, amp;, lt;, /TD> | Bal | 2.50 | V:7.0 | | 1.20 | | | | 低氫型焊條,用于鍛模、沖模 | Stellite706司太立焊絲,Stellite706司太立焊絲, , , , 焊接碳鋼及低合金鋼的焊芯, 一般都選用低碳鋼作為焊芯,并添加錳、硅、鉻、鎳等成分(詳見焊絲國(guó)家標(biāo)準(zhǔn)gb1300一77)。采用低碳的原因一方面是含碳量低時(shí)鋼絲塑性好,焊絲拉拔比較容易,另一方面可降低還原性氣體co含量,減少飛濺或氣孔,并可增高焊縫金屬凝固時(shí)的溫度,對(duì)仰焊有利。加入其他合金元素主要為保證焊縫的綜合機(jī)械性能,同時(shí)對(duì)焊接工藝性能及去除雜質(zhì),也有一定作用。, , , (5)藥皮類型:氧化鐵型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含多量氧化鐵和較多的錳鐵脫氧劑,熔深大,熔化速度快,焊接生產(chǎn)率較高,電弧穩(wěn)定,再引弧方便,立焊、仰焊較困難,飛濺稍大,焊縫抗熱裂性能較好,適用于中厚板焊接。由于電弧吹力大,適于野外操作。若藥皮中加入一定量的鐵粉,為鐵粉氧化鈦型。, 5。(crni)1~2字母,附加合金元素或焊條特性。, , 焊接碳鋼及低合金鋼的焊芯, 一般都選用低碳鋼作為焊芯,并添加錳、硅、鉻、鎳等成分(詳見焊絲國(guó)家標(biāo)準(zhǔn)gb1300一77)。采用低碳的原因一方面是含碳量低時(shí)鋼絲塑性好,焊絲拉拔比較容易,另一方面可降低還原性氣體co含量,減少飛濺或氣孔,并可增高焊縫金屬凝固時(shí)的溫度,對(duì)仰焊有利。加入其他合金元素主要為保證焊縫的綜合機(jī)械性能,同時(shí)對(duì)焊接工藝性能及去除雜質(zhì),也有一定作用。, , , 焊條 - 藥皮, , , 電焊條 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | Electrode | A-91 | 60%碳化鎢、其余為鋼管、A-91中的91為碳化鎢顆粒硬度 | 風(fēng)機(jī)攪拌機(jī)葉片、采礦、建筑易損件 | 鑄棒 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | W | Fe | Mo | Ni | Co | Mn | Stellite 1 | 53 | 2.50 | 29.50 | 1.20 | 12.50 | 3.00 | 1.00 | 3.00 | Bal | 1.00 | 閥座、軸承、刀口等 | Stellite 3 | 54 | 2.40 | 31.00 | 1.00 | 12.50 | 3.00 | | 3.00 | Bal | 1.00 | 針閥座、閥座、軋鋼導(dǎo)向輥 | Stellite 4 | 48 | 0.90 | 32.00 | 1.00 | 13.50 | 1.00 | 0.50 | 0.50 | Bal | 0.50 | 熱壓模、熱擠壓模、干電池工業(yè) | Stellite 6 | 43 | 1.20 | 29.00 | 1.20 | 4.50 | 3.00 | 1.00 | 3.00 | Bal | 1.00 | 發(fā)動(dòng)機(jī)氣門、高溫高壓閥門、渦輪機(jī)葉片 | Stellite 12 | 47 | 1.45 | 29.00 | 2.00 | 8.50 | 3.00 | 1.00 | 3.00 | Bal | 1.00 | 高溫高壓閥門、鋸齒、螺旋推桿等 | Stellite 20 | 54 | 2.45 | 32.50 | 1.00 | 17.00 | 3.00 | 1.00 | 3.00 | Bal | 0.50 | 軸承套筒、耐磨板 | Stellite 21 | 20 | 0.25 | 27.00 | 1.00 | 0.15 | 2.00 | 5.50 | 2.50 | Bal | 1.00 | 渦輪機(jī)葉片、各種液體閥、閥座、熱沖模等 | Stellite 31 | 33 | 0.50 | 25.50 | 1.00 | 7.50 | 2.00 | 1.00 | 10.50 | Bal | 1.00 | 燃?xì)鉁u輪葉片 | Stellite 190 | 58 | 3.20 | 26.00 | 1.00 | 14.00 | 5.00 | 1.00 | 3.00 | Bal | 1.00 | 石油鉆具 | Stellite 706 | 42 | 1.20 | 30.00 | 1.20 | | 2.00 | 5.00 | 2.00 | Bal | 1.00 | 發(fā)動(dòng)機(jī)氣門、高溫高壓閥門 | Stellite 712 | 50 | 2.00 | 29.00 | 2.00 | | 2.00 | 8.50 | 2.00 | Bal | 2.00 | 高溫高壓閥門、螺旋推桿 | Tribaloy 400 | 53 | 0.08 | 8.50 | 2.60 | | 1.50 | 28.50 | 1.50 | Bal | | 用于高溫強(qiáng)腐介質(zhì)中的閘閥、擠塑器 | Tribaloy 800 | 55 | 0.08 | 18.00 | 3.40 | | 1.50 | 28.50 | 1.50 | Bal | | 用于高溫強(qiáng)腐介質(zhì)中的閘閥、擠塑器 | Stellite F | 40 | 1.75 | 25.50 | 1.10 | | 1.15 | 0.60 | 22.50 | Bal | 0.30 | 內(nèi)燃機(jī)進(jìn)排氣閥 | Stellite706司太立焊絲,Stellite706司太立焊絲, 3。(50)二個(gè)數(shù)字,熔敷金屬?gòu)?qiáng)度或合金類型。, (5)藥皮類型:高纖維素鈉型 ‖藥皮主要成分 : 有機(jī)物15%以上,氧化鈦30%左右 ‖焊接電源:直流, , , , (8)藥皮類型:低氫鉀型 ‖藥皮主要成分 : 鈣、鎂的碳酸鹽和螢石 ‖焊接電源: 直流或交流, , 焊條藥皮類型特點(diǎn) http://www.wanhonghanjie.com, , , 焊條 - 藥皮, , , (3)熔渣的比重應(yīng)小于熔化金屬的比重,凝固溫度也應(yīng)稍低于金屬凝固溫度,渣殼應(yīng)易脫掉;, , 鑄棒 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | W | Fe | Mo | Ni | Co | Mn | B | Deloro 40 | 40 | 0.30 | 7.50 | 3.50 | | 2.20 | 0.10 | Bal | | 0.10 | 1.70 | 螺旋送料器、模芯、核工業(yè)中閥門的密封面 | Deloro 45 | 45 | 0.37 | 8.75 | 3.80 | | 4.00 | 0.10 | Bal | | 0.10 | 2.00 | 排氣閥密封面、柱塞 | Deloro 50 | 50 | 0.45 | 11.25 | 4.00 | | 2.80 | 0.10 | Bal | | 0.10 | 2.20 | 泵軸、紙漿刀、閥門、密封環(huán)、軸套 | Deloro 55 | 55 | 0.50 | 11.00 | 3.60 | | 4.50 | 0.10 | Bal | | 0.50 | 2.10 | 閥門、密封環(huán)、軸套 | Deloro 60 | 59 | 0.65 | 15.00 | 4.30 | | 4.00 | 0.10 | Bal | | 0.10 | 3.10 | 擠壓模、螺旋筒體、泵葉、柱塞 | Deloro 6325 | 56 | 0.50 | 16.00 | 4.00 | | 4.50 | 3.00 | Bal | | 0.10 | 3.50 | 耐蝕泵、軸、軸套 | Tribaloy 700 | 54 | 0.08 | 15.50 | 3.40 | | 1.50 | 32.50 | Bal | 1.50 | | | 核工業(yè)應(yīng)用抗蝕抗氧化抗輻射 | Nistelle B | 冷硬 | 0.10 | 1.00 | 1.00 | | 5.00 | 28.00 | Bal | 2.50 | 1.00 | | 高溫耐蝕密封環(huán) | Stellite706司太立焊絲, , , 編輯, , , , 高合金鋼以及鋁、銅、鑄鐵等其他金屬材料,其焊芯成分除要求與被焊金屬相近外,同樣也要控制雜質(zhì)的含量,并按工藝要求常加入某些特定的合金元素。http://www.wanhonghanjie.com, (4)具有摻合金和冶金處理作用;, , 5)鎳(ni)鎳對(duì)鋼的韌性有比較顯著的效果,一般低溫沖擊值要求較高時(shí),適當(dāng)摻入一些鎳。, , , 五、提高焊接生產(chǎn)率,減少飛濺。焊條藥皮具有使熔滴增加而減少飛濺的作用。焊條藥皮的熔點(diǎn)稍低于焊芯的焊點(diǎn),但因焊芯處于電弧的中心區(qū),溫度較高,所以焊芯先熔化,藥皮稍遲一點(diǎn)熔化。這樣,在焊條端頭形成一短段藥皮套管,加上電弧吹力的作用,使熔滴徑直射到熔池上,使之有利于仰焊和立焊。另外,在焊芯涂了藥皮后,電弧熱量更集中。同時(shí),由于減少了由飛濺引起的金屬損失,提高了熔敷系數(shù),也就提高了焊接生產(chǎn)率。另外,焊接過程中發(fā)塵量也會(huì)減少。http://www.wanhonghanjie.com, , , 合金元素對(duì)焊接影響 , 一、提高電弧燃燒的穩(wěn)定性。無藥皮的光焊條不容易引燃電弧。即使引燃了也不能穩(wěn)定地燃燒。在焊條藥皮中,一般含有鉀、鈉、鈣等電離電位低的物質(zhì),這可以提高電弧的穩(wěn)定性,保證焊接過程持續(xù)進(jìn)行。, , , (5)藥皮類型:氧化鐵型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含多量氧化鐵和較多的錳鐵脫氧劑,熔深大,熔化速度快,焊接生產(chǎn)率較高,電弧穩(wěn)定,再引弧方便,立焊、仰焊較困難,飛濺稍大,焊縫抗熱裂性能較好,適用于中厚板焊接。由于電弧吹力大,適于野外操作。若藥皮中加入一定量的鐵粉,為鐵粉氧化鈦型。, 焊條焊接時(shí),焊芯金屬占整個(gè)焊縫金屬的一部分。所以焊芯的化學(xué)成分,直接影響焊縫的質(zhì)量。因此,作為焊條芯用的鋼絲都單獨(dú)規(guī)定了它的牌號(hào)與成分。如果用于埋弧自動(dòng)焊、電渣焊、氣體保護(hù)焊、氣焊等熔焊方法作填充金屬時(shí),則稱為焊絲。http://www.wanhonghanjie.com, (3)藥皮類型:鈦鈣型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含氧化鈦30%以上,鈣、鎂的碳酸鹽20%以下,焊條工藝性能良好,熔渣流動(dòng)性好,熔深一般,電弧穩(wěn)定,焊縫美觀,脫渣方便,適用于全位置焊接,如j422即屬此類型,是目前碳鋼焊條中使用最廣泛的一種焊條。, , , 焊條焊接時(shí),焊芯金屬占整個(gè)焊縫金屬的一部分。所以焊芯的化學(xué)成分,直接影響焊縫的質(zhì)量。因此,作為焊條芯用的鋼絲都單獨(dú)規(guī)定了它的牌號(hào)與成分。如果用于埋弧自動(dòng)焊、電渣焊、氣體保護(hù)焊、氣焊等熔焊方法作填充金屬時(shí),則稱為焊絲。http://www.wanhonghanjie.com, |