管狀焊絲 | 焊劑 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | Mo | Mn | Fe | W | Ni | V | B | 其他 | Delcrome 103 | 107 | 54 | 5.15 | 27.50 | 1.50 | | 2.50 | Bal | | | | | | 磨煤輥 | Multipass 104 | 431 | 28 | 0.25 | 1.20 | 1.50 | | 3.00 | Bal | | | | | | 軋輥等堆焊過渡層及軸的修復(fù) | Multipass 105 | 431 | 45 | 0.50 | 4.00 | 1.10 | 0.50 | 2.75 | Bal | | | | | | 拖拉機(jī)惰輪、礦車輪、導(dǎo)輥 | Multipass 107 | 431 | 37 | 0.35 | 2.70 | 1.20 | 0.25 | 2.70 | Bal | | | | | | 卷筒、拖拉機(jī)惰輪、礦車輪 | Multipass 109 | 260 | | 0.45 | 3.10 | 0.60 | | 0.60 | Bal | | 0.5 | | | | 管模、鋁軋輥等 | Multipass 224 | 107 | 46 | 0.45 | 5.50 | 0.65 | 1.10 | 1.80 | Bal | 1.50 | | | | | 各類軋輥及連鑄第3區(qū)輥 | Multipass 224H | 107 | 53 | 0.55 | 6.50 | 0.65 | 1.10 | 1.80 | Bal | 1.50 | | | | 1.0 | 熱軋工作輥、支撐輥、開坯輥 | Multipass 224HC | 107 | 58 | 0.75 | 7.70 | 0.75 | 1.80 | 1.70 | Bal | 2.60 | | | | 1.0 | 支撐輥、校直輥、助卷輥 | Multipass 225 | 107 | 59 | 0.90 | 6.00 | 0.50 | 1.20 | 0.80 | Bal | 8.60 | | | | | 熱軋支撐輥 | Multipass 235 | 107 | 60 | 0.45 | 9.00 | | 2.20 | 0.70 | Bal | 8.40 | Co:10.5 | 0.30 | | | 熱軋支撐輥 | Multipass 236 | | | 0.28 | 3.10 | 0.70 | 2.00 | 0.70 | Bal | 1.90 | | 0.65 | | | 鋼管成型輥 | Multipass 915 | 107 | 60 | 1.20 | 20.00 | 0.50 | | 0.70 | Bal | | | | 4.00 | | 高速磨打擊板等耐強(qiáng)沖擊,強(qiáng)磨粒磨損場合 | Delstain 414-S | 260 | 40 | 0.20 | 14.00 | 0.50 | 1.00 | 1.40 | Bal | | 4.20 | | | | 連鑄輥等耐磨耐高溫場合 | Delstain 420 | 260 | 46 | 0.40 | 13.00 | 0.50 | | 1.40 | Bal | | | | | | 一般軋鋼輥、剎車鼓、卷輥 | Delstain 423 | 107 | 45 | 0.33 | 13.50 | 0.50 | 1.20 | 1.50 | Bal | | 2.50 | 0.20 | | | 連鑄機(jī)輥、熱軋輥堆焊 | Delstain 424H | 260 | 49 | 0.40 | 12.00 | 0.50 | 0.90 | 2.20 | Bal | | 1.40 | | | | 有色工作輥的堆焊 | Delstain 430 | 260 | | 0.10 | 19.00 | 0.50 | | 0.70 | Bal | | 0.60 | | | | 連鑄輥等耐磨耐高溫場合 | Delcrome 911 | 107 | 57 | 6.60 | 36.50 | 0.40 | | 0.40 | Bal | | | | | | 磨煤輥堆焊 | Delcrome 100HD | 107 | 57 | 6.80 | 29.00 | 1.00 | | 2.0 | Bal | | | | | Zr:0.45 | 磨煤輥等耐中等沖擊,強(qiáng)磨粒磨損場合 | STW 101 | 431 | HB:250 | 0.25 | 1.35 | 0.55 | 0.60 | 1.35 | Bal | | | 0.25 | | | 碳鋼、低合金鋼部件修復(fù) | STW 102 | 431 | 36 | 0.25 | 2.95 | 0.55 | 1.00 | 1.00 | Bal | | 1.35 | 0.10 | | | 碳鋼、低合金鋼部件修復(fù) | STW 103 | | | 0.35 | 3.00 | 0.70 | 2.00 | 1.40 | Bal | | | 0.60 | | | 碳鋼、低合金鋼部件修復(fù) | STE308L-16司太立焊絲,STE308L-16司太立焊絲, 焊條的牌號 , , , (5)藥皮類型:氧化鐵型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含多量氧化鐵和較多的錳鐵脫氧劑,熔深大,熔化速度快,焊接生產(chǎn)率較高,電弧穩(wěn)定,再引弧方便,立焊、仰焊較困難,飛濺稍大,焊縫抗熱裂性能較好,適用于中厚板焊接。由于電弧吹力大,適于野外操作。若藥皮中加入一定量的鐵粉,為鐵粉氧化鈦型。, 編輯, 人們在實(shí)踐過程中發(fā)現(xiàn)如果在光焊條外面涂一層由各種礦物等組成的藥皮,能使電弧燃燒穩(wěn)定,焊縫質(zhì)量得到提高,這種焊條叫藥皮焊條。隨著工業(yè)技術(shù)的不斷發(fā)展,人們創(chuàng)制出了廣泛應(yīng)用的優(yōu)質(zhì)厚藥皮焊條。http://www.wanhonghanjie.com, , , 焊條牌號的編制方法 ,, 合金元素對焊接影響 , , , 5)鎳(ni)鎳對鋼的韌性有比較顯著的效果,一般低溫沖擊值要求較高時,適當(dāng)摻入一些鎳。, , 管狀焊絲 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | Tungsmooth 60 | A-91 | 60%碳化鎢、其余為鋼管、A-91中的91為碳化鎢顆粒硬度 | 風(fēng)機(jī)攪拌機(jī)葉片、采礦、建筑易損件 | 管狀焊絲 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | Mo | Mn | Fe | Ni | Al | 其他 | Delcrome 11-o | 50 | 3.20 | 14.50 | 0.90 | 0.45 | 1.40 | Bal | | | | 破碎機(jī)錘頭、挖土機(jī)齒 | Delcrome 94-o | 57 | 3.20 | 24.50 | 0.70 | | 0.80 | Bal | 2.80 | | | 筑路機(jī)零件、攪拌葉片 | Delcrome 100-o | 57 | 3.80 | 26.50 | 1.40 | 1.30 | 1.90 | Bal | | | | 磨煤輥 | Delcrome 100HC-o | 60 | 5.50 | 26.50 | 2.40 | 1.30 | 1.90 | Bal | | | | 磨煤輥、破碎輥 | Delcrome 117-o | 43 | 2.30 | 10.50 | 1.30 | 1.50 | 1.50 | Bal | zr:0.40 | | Cu:0.40 | 破碎輥、錘頭 | Delcrome 150-o | 58 | 2.20 | 7.00 | | 2.00 | 1.00 | Bal | V:0.20 | | Ti:7.00 | 水泥擠壓輥、錘頭、農(nóng)具 | Delcrome 945-o | 57 | 5.00 | 21.50 | 0.70 | 4.50 | 0.70 | Bal | W:2.00 | | Nb:7.00 | 高爐加料槽板、閘閥 | Build up | 35 | 0.15 | 0.90 | 0.90 | 0.40 | 1.80 | Bal | | | | 碳鋼、低合金鋼恢復(fù)尺寸如齒輪、錘頭 | Ni-Mang-o | 冷硬 | 0.85 | 3.00 | 0.50 | | 14.00 | Bal | 3.00 | | | 破碎機(jī)輥、顎板、挖泥機(jī)刀片 | Sta-Mang-o | 冷硬 | 0.10 | 10.00 | 0.50 | 0.80 | 15.50 | Bal | 0.85 | | | 破碎機(jī)、鐵鏟、鐵路道岔 | Multipass 4-o | 34 | 0.15 | 0.70 | 1.10 | 0.30 | 2.00 | Bal | | | | 碳鋼、低合金鋼部件修復(fù) | Multipass 5-o | 44 | 0.10 | 2.30 | 0.30 | 0.50 | 1.40 | Bal | | | | 拖拉機(jī)惰輪、起重機(jī)輪 | Multipass 1265-g | 55 | 0.65 | 5.50 | 0.50 | 1.50 | 1.00 | Bal | W:1.50 | | V:0.30 | 冷沖壓模 | Delcrome 90G | 48 | 2.40 | 24.00 | 0.60 | | 0.90 | Bal | | | | 鏟斗齒、排氣葉、提升斗 | Delcrome 94G | 52 | 3.00 | 28.00 | 1.40 | | 1.20 | Bal | B:0.80 | | | 鏟斗齒、攪拌機(jī)、破碎輥 | Mulitpass 106 | | 0.10 | | 0.90 | 5.20 | 1.40 | Bal | 5.20 | | | 管模,鋁軋輥等 | Delcrome 165 | 62 | 6.80 | 30.00 | 3.00 | 0.50 | 0.50 | Bal | W:4.20 | | Nb:2.60 | 磨煤 輥等耐中等沖擊,強(qiáng)磨粒磨損場合 | Delstain 414N-o | 47 | 0.20 | 14.00 | 0.50 | 1.00 | 1.30 | Bal | 4.20 | | N:0.22 | 連鑄輥等耐磨耐高溫場合 | Delstain 431 | 33 | 0.40 | 17.50 | 0.50 | | 1.20 | Bal | | | | 連鑄輥等耐磨耐高溫場合 | Delcrome 103HD | 60 | 5.60 | 30.00 | 1.10 | 0.80 | 1.20 | Bal | | | Cu:0.10 | 磨煤輥等 | Stellarc 420 | 430(HV) | 0.3 | 13 | 1 | | 1 | Bal | | | | 具有一定的耐大氣腐蝕及良好的耐磨性,可用于一般機(jī)械零件的修復(fù)、保護(hù) | Stellarc 430 | 400(HV) | 0.7 | 17 | 1 | 0.5 | 1 | Bal | | | | 具有一定的耐大氣腐蝕及良好的耐磨性,可用于一般機(jī)械零件的修復(fù)、保護(hù) | Stellarc 316 | 240(HV) | 0.08 | 18 | 0.7 | 2.5 | 1 | Bal | 13 | | | 具有一定的耐大氣腐蝕及良好的耐磨性,可用于一般機(jī)械零件的修復(fù)、保護(hù) | Stellarc 100 | 660(HV) | 5 | 28 | 0.5 | | 1 | Bal | | | | 具有優(yōu)良的耐磨性 | Stellarc 250 | | | 1 | 0.5 | 0.5 | 1 | Bal | | | WC:50 | 風(fēng)機(jī)、風(fēng)管、煙道內(nèi)壁 | Stellarc 45 | 400(HV) | | 45 | | | | | Bal | | | 風(fēng)機(jī)、風(fēng)管、煙道內(nèi)壁 | Stellarc 95 | 480(HV) | | | | | | | Bal | 5 | | 打底涂層 | Stellarc 625 | 260(HV) | 0.08 | 21 | | 9 | | 5 | Bal | 5 | Nb+Ta:4 | 優(yōu)異的抗高溫腐蝕及耐磨介質(zhì) | Stellarc 276 | | 0.08 | 16 | | 16 | | 5 | Bal | | W:4 | 耐腐蝕性能優(yōu)異,能抗硫酸、鹽酸或其他有機(jī)酸的腐蝕 | STE308L-16司太立焊絲,STE308L-16司太立焊絲, 3)硅(si )硅也是一種較好的合金劑,在鋼中加入適量的硅能提高鋼的屈服強(qiáng)度、彈性及抗酸性能;若含量過高,則降低塑性和韌性。在焊接過程中,硅也具有較好的脫氧能力,與氧形成二氧化硅,但它會提高渣的粘度,易促進(jìn)非金屬夾雜物生成。, (4)藥皮類型:鈦鐵礦型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含鈦鐵礦305,焊條熔化速度快,熔渣流動性好,熔深較深,脫渣容易,焊波整齊,電弧穩(wěn)定,平焊、平角焊工藝性能較好,立焊稍次,焊縫有較好的抗裂性。, , , 三、保證焊縫脫氧、去硫磷雜質(zhì)。焊接過程中雖然進(jìn)行了保護(hù),但仍難免有少量氧進(jìn)入熔池,使金屬及合金元素氧化,燒損合金元素,降低焊縫質(zhì)量。因此,需要在焊條藥皮中加入還原劑(如錳、硅、鈦、鋁等),使已進(jìn)入熔池的氧化物還原。http://www.wanhonghanjie.com, (4)具有摻合金和冶金處理作用;, , , , 4)鉻(cr)鉻能夠提高鋼的硬度、耐磨性和耐腐蝕性。對于低碳鋼來說,鉻便是一種偶然的雜質(zhì)。鉻的主要冶金特征是易于急劇氧化,形成難熔的氧化物三氧化二鉻(cr203),從而增加了焊縫金屬夾雜物的可能性。三氧化二鉻過渡到熔渣后,能使熔渣粘度提高,流動性降低。, 五、提高焊接生產(chǎn)率,減少飛濺。焊條藥皮具有使熔滴增加而減少飛濺的作用。焊條藥皮的熔點(diǎn)稍低于焊芯的焊點(diǎn),但因焊芯處于電弧的中心區(qū),溫度較高,所以焊芯先熔化,藥皮稍遲一點(diǎn)熔化。這樣,在焊條端頭形成一短段藥皮套管,加上電弧吹力的作用,使熔滴徑直射到熔池上,使之有利于仰焊和立焊。另外,在焊芯涂了藥皮后,電弧熱量更集中。同時,由于減少了由飛濺引起的金屬損失,提高了熔敷系數(shù),也就提高了焊接生產(chǎn)率。另外,焊接過程中發(fā)塵量也會減少。http://www.wanhonghanjie.com, , , , , 電焊條 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | W | Fe | Mo | Ni | Co | Mn | B | Cu | 其他 | Stellite 1 | 48 | 2.20 | 29.00 | 2.00 | 14.00 | 3.00 | 0.50 | 3.00 | Bal | 1.00 | | | | 閥座、軸承、刀口等 | Stellite 6 | 40 | 1.00 | 29.00 | 1.00 | 4.50 | 3.00 | 0.50 | 3.00 | Bal | 1.00 | | | | 發(fā)動機(jī)氣門、高溫高壓閥門、渦輪機(jī)葉片 | Stellite 12 | 44 | 1.30 | 29.00 | 1.00 | 9.00 | 3.00 | 0.50 | 3.00 | Bal | 1.00 | | | | 高溫高壓閥門、鋸齒、螺旋推桿等 | Stellite 21 | 23 | 0.30 | 28.00 | 1.00 | | 2.50 | 5.50 | 2.50 | Bal | 2.00 | | | | 渦輪機(jī)葉片、閥座、熱沖模 | Stellite 25 | 冷硬 | 0.15 | 20.00 | 1.00 | 14.00 | 3.00 | 0.50 | 10.00 | Bal | 1.50 | | | | 高溫耐蝕密封面、擠壓模 | Nistelle C | | 0.10 | 17.00 | | 5.00 | 6.00 | 17.00 | Bal | | | | | | 高溫耐蝕密封環(huán) | Ni-Mang | 冷硬 | 0.60 | 2.70 | 0.20 | | Bal | | 3.70 | | 13.50 | | | | 錘式破碎機(jī)、高錳鋼部件焊接 | STE 308-16 | | 0.08 | 19.50 | 0.90 | | Bal | 0.50 | 10.00 | | 0.80 | | 0.50 | | 用于焊接Cr18Ni8不銹鋼 | STE 308L-16 | | 0.03 | 19.50 | 0.90 | | Bal | 0.50 | 10.00 | | 0.80 | | 0.50 | | 用于焊接超低碳Cr18Ni8不銹鋼 | STE 309-16 | | 0.15 | 23.50 | 0.90 | | Bal | 0.50 | 13.00 | | 0.80 | | 0.50 | | 用于焊接Cr22Nil2不銹鋼及用于不銹鋼與低碳鋼或低合金鋼之間的焊接 | STE 309L-16 | | 0.02 | 23.50 | 0.90 | | Bal | 0.50 | 13.00 | | 0.80 | | 0.50 | | 打底層焊接,異種鋼焊接,易產(chǎn)生裂紋部位的焊接 | STE 309Mo-16 | | 0.12 | 23.50 | 0.90 | | Bal | 2.50 | 13.00 | | 0.80 | | | | 用于焊接Cr22Nil2-Mo不銹鋼 | STE 309MoL-16 | | 0.03 | 23.50 | 0.90 | | Bal | 2.50 | 13.00 | | 0.80 | | | | 用于焊接超低碳Cr22Nil2Mo不銹鋼 | STE 310-16 | | 0.20 | 26.50 | 0.75 | | Bal | 0.50 | 21.50 | | 1.50 | | 0.50 | | 用于焊接Cr25Ni20不銹鋼 | STE 310Mo-16 | | 0.08 | 26.50 | 0.75 | | Bal | 2.50 | 21.00 | | 1.20 | | 0.50 | | 耐硫酸腐蝕、抗裂性、高溫性能優(yōu)良 | STE 316-16 | | 0.05 | 18.50 | 0.90 | | Bal | 2.50 | 12.50 | | 0.80 | | 0.50 | | 用于焊接Cr18Ni12Mo2不銹鋼 | STE 316L-16 | | 0.03 | 18.50 | 0.90 | | Bal | 2.50 | 12.50 | | 0.80 | | 0.50 | | 用于焊接超低碳Cr18Ni12Mo2不銹鋼 | STE 316LF | | 0.02 | 18.00 | 0.75 | | Bal | 2.70 | 16.00 | | 2.00 | | 0.50 | | 耐尿素腐蝕性優(yōu)良 | STE 347-16 | | 0.08 | 19.50 | 0.50 | | Bal | 0.50 | 10.00 | | 0.80 | | 0.50 | 8xc-1.00 | 用于焊接Cr18Ni8含鈮或鈦的不銹鋼 | STE 997 | 56 | 0.60 | 5.50 | 0.80 | | Bal | 4.00 | W:7.0 | | 0.70 | | | | 低氫型高速鋼焊條 | D 287 | 40 | 0.10 | 14.00 | 0.50 | | Bal | 1.00 | 5.00 | | 0.50 | | | | 水泵、水輪機(jī)部件 | D 907 | 冷硬 | 0.20 | 21.00 | 1.00 | 2.50 | Bal | 3.00 | | 20.00 | 1.50 | | | | 熱剪刀片 | Delcrome 90sc | 52 | 2.10 | 26.00 | 1.10 | | Bal | | | | 0.90 | | | | 挖掘設(shè)備、破碎輥、錘 | Delcrome 91 | 55 | 3.00 | 31.00 | 0.60 | | Bal | 1.30 | | | 0.90 | | | | 破碎機(jī)輥、錘頭、泥漿泵部件 | Delcrome 94 | 53 | 3.00 | 31.00 | 0.40 | | Bal | 1.30 | | | 0.90 | | | | 鏟斗齒、攪拌機(jī)、挖掘采礦設(shè)備 | Delcrome 945 | 58 | 5.40 | 1.20 | | Bal | | | | 1.00 | | | Nb:5.00 | 耐侵蝕、抗高溫腐蝕及磨損場合 | Delcrome 23 | 44 | 0.20 | 5.50 | 1.00 | &n, bsp;&, amp;, lt;, /TD> | Bal | 2.50 | V:7.0 | | 1.20 | | | | 低氫型焊條,用于鍛模、沖模 | STE308L-16司太立焊絲,STE308L-16司太立焊絲, 5。(crni)1~2字母,附加合金元素或焊條特性。, , (6)藥皮類型:纖維素型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含15%以上的有機(jī)物,30%左右的氧化鈦,焊接工藝性能良好,電弧穩(wěn)定,電弧吹力大,熔深大,熔渣少,脫渣容易。可作立向下焊、深熔焊或單面焊雙面成形焊接。立、仰焊工藝性好。適用于薄板結(jié)構(gòu)、油箱管道、車輛殼體等焊接。隨藥皮中穩(wěn)弧劑、黏結(jié)劑含量變化,分為高纖維素鈉型(采用直流反接)、高纖維素鉀型兩類, , , , , 以結(jié)構(gòu)鋼為例:牌號,編制法。結(jié)xxx,結(jié)為結(jié)構(gòu)鋼焊條,第3個數(shù)字,代表藥皮類型,焊接電流要求,第1、2數(shù):代表焊縫金屬抗拉強(qiáng)度 。, 焊條就是涂有藥皮的供焊條電弧焊使用的熔化電極,它是由藥皮和焊芯兩部分組成的。在焊條前端藥皮有45°左右的倒角,這是為了便于引弧。在尾部有一段裸焊芯,約占焊條總長1/16,便于焊鉗夾持并有利于導(dǎo)電。焊條的直徑實(shí)際上是指焊芯直徑)通常為2、2.5、3.2或3、4、5或6mm等幾種規(guī)格,最常用的是小3.2、小4、小5三種,其長度“l(fā)”一般在200~550 mm之間。, , 四、為焊縫補(bǔ)充合金元素。由于電弧的高溫作用,焊縫金屬的合金元素會被蒸發(fā)燒損,使焊縫的機(jī)械性能降低。因此,必須通過藥皮向焊縫加入適當(dāng)?shù)暮辖鹪兀詮浹a(bǔ)合金元素的燒損,保證或提高焊縫的機(jī)械性能。對有些合金鋼的焊接,也需要通過藥皮向焊縫滲入合金,使焊縫金屬能與母材金屬成分相接近,機(jī)械性能趕上甚至超過基本金屬。, , (8)藥皮類型:石墨型 電源種類:直流或交流 主要特點(diǎn):藥皮中含有多量石墨,通常用于鑄鐵或堆焊焊條。采用低碳鋼焊芯時,焊接工藝性能較差,飛濺較多,煙霧較大,熔渣少,適于平焊。采用有色金屬焊芯時,能改善其工藝性能,但電流不易過大。, 1。(chh) 二個字母,中國航海產(chǎn)品代號。, 2)錳(mn)錳在鋼中是一種較好的合金劑,隨著錳含量的增加,其強(qiáng)度和韌性會有所提高。在焊接過程中,錳也是一種較好的脫氧劑,能減少焊縫中氧的含量。錳與硫化合形成硫化錳浮于熔渣中,從而減少焊縫熱裂紋傾向。因此一般碳素結(jié)構(gòu)鋼焊芯的含錳量為0. 30%~0. 55%,焊接某些特殊用途的鋼絲,其含錳量高達(dá)1 .70%一2. 10%。, 電焊條 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | Electrode | A-91 | 60%碳化鎢、其余為鋼管、A-91中的91為碳化鎢顆粒硬度 | 風(fēng)機(jī)攪拌機(jī)葉片、采礦、建筑易損件 | 鑄棒 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | W | Fe | Mo | Ni | Co | Mn | Stellite 1 | 53 | 2.50 | 29.50 | 1.20 | 12.50 | 3.00 | 1.00 | 3.00 | Bal | 1.00 | 閥座、軸承、刀口等 | Stellite 3 | 54 | 2.40 | 31.00 | 1.00 | 12.50 | 3.00 | | 3.00 | Bal | 1.00 | 針閥座、閥座、軋鋼導(dǎo)向輥 | Stellite 4 | 48 | 0.90 | 32.00 | 1.00 | 13.50 | 1.00 | 0.50 | 0.50 | Bal | 0.50 | 熱壓模、熱擠壓模、干電池工業(yè) | Stellite 6 | 43 | 1.20 | 29.00 | 1.20 | 4.50 | 3.00 | 1.00 | 3.00 | Bal | 1.00 | 發(fā)動機(jī)氣門、高溫高壓閥門、渦輪機(jī)葉片 | Stellite 12 | 47 | 1.45 | 29.00 | 2.00 | 8.50 | 3.00 | 1.00 | 3.00 | Bal | 1.00 | 高溫高壓閥門、鋸齒、螺旋推桿等 | Stellite 20 | 54 | 2.45 | 32.50 | 1.00 | 17.00 | 3.00 | 1.00 | 3.00 | Bal | 0.50 | 軸承套筒、耐磨板 | Stellite 21 | 20 | 0.25 | 27.00 | 1.00 | 0.15 | 2.00 | 5.50 | 2.50 | Bal | 1.00 | 渦輪機(jī)葉片、各種液體閥、閥座、熱沖模等 | Stellite 31 | 33 | 0.50 | 25.50 | 1.00 | 7.50 | 2.00 | 1.00 | 10.50 | Bal | 1.00 | 燃?xì)鉁u輪葉片 | Stellite 190 | 58 | 3.20 | 26.00 | 1.00 | 14.00 | 5.00 | 1.00 | 3.00 | Bal | 1.00 | 石油鉆具 | Stellite 706 | 42 | 1.20 | 30.00 | 1.20 | | 2.00 | 5.00 | 2.00 | Bal | 1.00 | 發(fā)動機(jī)氣門、高溫高壓閥門 | Stellite 712 | 50 | 2.00 | 29.00 | 2.00 | | 2.00 | 8.50 | 2.00 | Bal | 2.00 | 高溫高壓閥門、螺旋推桿 | Tribaloy 400 | 53 | 0.08 | 8.50 | 2.60 | | 1.50 | 28.50 | 1.50 | Bal | | 用于高溫強(qiáng)腐介質(zhì)中的閘閥、擠塑器 | Tribaloy 800 | 55 | 0.08 | 18.00 | 3.40 | | 1.50 | 28.50 | 1.50 | Bal | | 用于高溫強(qiáng)腐介質(zhì)中的閘閥、擠塑器 | Stellite F | 40 | 1.75 | 25.50 | 1.10 | | 1.15 | 0.60 | 22.50 | Bal | 0.30 | 內(nèi)燃機(jī)進(jìn)排氣閥 | STE308L-16司太立焊絲,STE308L-16司太立焊絲, 焊條焊接時,焊芯金屬占整個焊縫金屬的一部分。所以焊芯的化學(xué)成分,直接影響焊縫的質(zhì)量。因此,作為焊條芯用的鋼絲都單獨(dú)規(guī)定了它的牌號與成分。如果用于埋弧自動焊、電渣焊、氣體保護(hù)焊、氣焊等熔焊方法作填充金屬時,則稱為焊絲。http://www.wanhonghanjie.com, , 2)錳(mn)錳在鋼中是一種較好的合金劑,隨著錳含量的增加,其強(qiáng)度和韌性會有所提高。在焊接過程中,錳也是一種較好的脫氧劑,能減少焊縫中氧的含量。錳與硫化合形成硫化錳浮于熔渣中,從而減少焊縫熱裂紋傾向。因此一般碳素結(jié)構(gòu)鋼焊芯的含錳量為0. 30%~0. 55%,焊接某些特殊用途的鋼絲,其含錳量高達(dá)1 .70%一2. 10%。, 三、保證焊縫脫氧、去硫磷雜質(zhì)。焊接過程中雖然進(jìn)行了保護(hù),但仍難免有少量氧進(jìn)入熔池,使金屬及合金元素氧化,燒損合金元素,降低焊縫質(zhì)量。因此,需要在焊條藥皮中加入還原劑(如錳、硅、鈦、鋁等),使已進(jìn)入熔池的氧化物還原。http://www.wanhonghanjie.com, , 此外,對于藥皮中含有多量鐵粉的焊條,可以稱為鐵粉焊條。這時,按照相應(yīng)焊條藥皮的主要成分,又可分為鐵粉鈦型、鐵粉鈦鐵礦型、鐵粉氧化鐵型、鐵粉低氫型等,構(gòu)成了鐵粉焊條系列。, , 1.chh:中國航海產(chǎn)品代號http://www.wanhonghanjie.com, 3)硅(si )硅也是一種較好的合金劑,在鋼中加入適量的硅能提高鋼的屈服強(qiáng)度、彈性及抗酸性能;若含量過高,則降低塑性和韌性。在焊接過程中,硅也具有較好的脫氧能力,與氧形成二氧化硅,但它會提高渣的粘度,易促進(jìn)非金屬夾雜物生成。, , , , , , , 鑄棒 | 硬度 | 化學(xué)成分(重量%) | 典型用途 | C | Cr | Si | W | Fe | Mo | Ni | Co | Mn | B | Deloro 40 | 40 | 0.30 | 7.50 | 3.50 | | 2.20 | 0.10 | Bal | | 0.10 | 1.70 | 螺旋送料器、模芯、核工業(yè)中閥門的密封面 | Deloro 45 | 45 | 0.37 | 8.75 | 3.80 | | 4.00 | 0.10 | Bal | | 0.10 | 2.00 | 排氣閥密封面、柱塞 | Deloro 50 | 50 | 0.45 | 11.25 | 4.00 | | 2.80 | 0.10 | Bal | | 0.10 | 2.20 | 泵軸、紙漿刀、閥門、密封環(huán)、軸套 | Deloro 55 | 55 | 0.50 | 11.00 | 3.60 | | 4.50 | 0.10 | Bal | | 0.50 | 2.10 | 閥門、密封環(huán)、軸套 | Deloro 60 | 59 | 0.65 | 15.00 | 4.30 | | 4.00 | 0.10 | Bal | | 0.10 | 3.10 | 擠壓模、螺旋筒體、泵葉、柱塞 | Deloro 6325 | 56 | 0.50 | 16.00 | 4.00 | | 4.50 | 3.00 | Bal | | 0.10 | 3.50 | 耐蝕泵、軸、軸套 | Tribaloy 700 | 54 | 0.08 | 15.50 | 3.40 | | 1.50 | 32.50 | Bal | 1.50 | | | 核工業(yè)應(yīng)用抗蝕抗氧化抗輻射 | Nistelle B | 冷硬 | 0.10 | 1.00 | 1.00 | | 5.00 | 28.00 | Bal | 2.50 | 1.00 | | 高溫耐蝕密封環(huán) | STE308L-16司太立焊絲, 合金元素對焊接影響 , , (4)藥皮類型:氧化鐵型 ‖藥皮主要成分 :多量氧化鐵及較多的錳鐵脫氧劑 ‖焊接電源: 直流或交流, , , 4。(7)一個數(shù)字,藥皮類型及電流種類。, , 二、保護(hù)焊接熔池。焊接過程中,空氣中的氧、氮及水蒸氣浸入焊縫,會給焊縫帶來不利的影響。不僅形成氣孔,而且還會降低焊縫的機(jī)械性能,甚至導(dǎo)致裂紋。而焊條藥皮熔化后,產(chǎn)生的大量氣體籠罩著電弧和熔池,會減少熔化的金屬和空氣的相互作用。焊縫冷卻時,熔化后的藥皮形成一層熔渣,覆蓋在焊縫表面,保護(hù)焊縫金屬并使之緩慢冷卻、減少產(chǎn)生氣孔的可能性。, (8)藥皮類型:低氫鉀型 ‖藥皮主要成分 : 鈣、鎂的碳酸鹽和螢石 ‖焊接電源: 直流或交流, (4)藥皮類型:鈦鐵礦型 電源種類: 直流或交流 主要特點(diǎn):藥皮中含鈦鐵礦305,焊條熔化速度快,熔渣流動性好,熔深較深,脫渣容易,焊波整齊,電弧穩(wěn)定,平焊、平角焊工藝性能較好,立焊稍次,焊縫有較好的抗裂性。, (5)適應(yīng)各種位置的焊接。, , , 焊條中被藥皮包覆的金屬芯稱為焊芯。焊芯一般是一根具有一定長度及直徑的鋼絲。焊接時,焊芯有兩個作用:一是傳導(dǎo)焊接電流,產(chǎn)生電弧把電能轉(zhuǎn)換成熱能,二是焊芯本身熔化作為填充金屬與液體母材金屬熔合形成焊縫。, 七、焊條藥皮類型及主要特點(diǎn)。按照藥皮的主要成分可以確定焊條的藥皮類型。由于藥皮配方組成不同,致使各種藥皮類型焊條的熔渣特性、焊接工藝性能以及焊縫金屬力學(xué)性能有很大差別。即使是同一類型藥皮,但不同牌號的焊條也因?yàn)樗幤こ煞趾团浔炔煌笚l的工藝性能等也會出現(xiàn)明顯的差別。, , (3)藥皮類型:鈦鐵礦型 ‖藥皮主要成分 :鈦鐵礦≥30% ‖焊接電源:直流或交流, , , , , 焊條藥皮是指涂在焊芯表面的涂料層。藥皮在焊接過程中分解熔化后形成氣體和熔渣,起到機(jī)械保護(hù)、冶金處理、改善工藝性能的作用。藥皮的組成物有:礦物類(如大理石、氟石等)、鐵合金和金屬粉類(如錳鐵、鈦鐵等)、有機(jī)物類(如木粉、淀粉等)、化工產(chǎn)品類(如鈦***、水玻璃等)。焊條藥皮是決定焊縫質(zhì)量的重要因素,在焊接過程中有以下幾方面的作用:, , (4)具有摻合金和冶金處理作用;, , |